Thickness dependence of the terahertz response in 〈110〉-oriented GaAs crystals for electro-optic sampling at 1.55 µm

Zhenyu Zhao, Andre Schwagmann, Frank Ospald, Daniel C. Driscoll, Hong Lu, Arthur C. Gossard, and Jurgen H. Smet  »View Author Affiliations


Optics Express, Vol. 18, Issue 15, pp. 15956-15963 (2010)
http://dx.doi.org/10.1364/OE.18.015956


View Full Text Article

Acrobat PDF (883 KB)





Browse Journals / Lookup Meetings

Browse by Journal and Year


   


Lookup Conference Papers

Close Browse Journals / Lookup Meetings

Article Tools

Share
Citations

Abstract

We experimentally study the thickness dependence of the terahertz (THz) response in 〈110〉-oriented GaAs crystals for free space electro-optic sampling at 1.55 µm. The THz response bandwidths are analyzed and simulated under phase-matching condition with a model frequency response function. The results indicate that the detection bandwidth increases from 2 THz to 3 THz when the thickness of GaAs is reduced from 2 mm to 1 mm. Below 1 mm, the detected bandwidth is increasingly limited by the emitter characteristics and the finite probe pulse duration. The broadest bandwidth in experiment reaches 3.3 THz when using a 0.2 mm thick crystal, while it exceeds 5 THz in theory. The THz response sensitivity was studied experimentally and modeled taking into account the absorption of the THz radiation in the GaAs crystal. While absorption was found to be negligible for the crystal thickness range studied here, strong saturation is predicted theoretically for crystal thicknesses exceeding 5 mm.

© 2010 Optical Society of America

1. Introduction

The rapidly growing demand for low-cost compact THz spectrometers has given rise to a strong interest in the development of coherent detection schemes with 1.55 µm femtosecond fiber lasers [1

1. B. Sartorius, H. Roehle, H. Künzel, J. Böttcher, M. Schlak, D. Stanze, H. Venghaus, and M. Schell, “All-fiber terahertz time-domain spectrometer operating at 1.5 µm telecom wavelengths,” Opt. Express 16, 9565–9570 (2008). [CrossRef] [PubMed]

, 2

2. A. Schneider, M. Stillhart, and P. Günter, “High efficiency generation and detection of terahertz pulses using laser pulses at telecommunication wavelengths,” Opt. Express 14, 5376–5384 (2006). [CrossRef] [PubMed]

]. Photoconductive antennas based on In0.53Ga0.47As compounds [3–5

3. J. Mangeney and P. Crozat, “Ion-irradiated In0.53Ga0.47As photoconductive antennas for THz generation and detection at 1.55 µm wavelength,” C. R. Phys. 9, 142–152 (2008). [CrossRef]

] have been studied since their intrinsic bandgap (E gap = 0.74 eV) suits this optical excitation wavelength. Free space electro-optic sampling (FSEOS) is an alternative detection scheme that is based on the Pockels effect and allows for measuring transient electromagnetic radiation with extremely high temporal resolution [6

6. Y. Cai, I. Brener, J. Lopata, J. Wynn, L. Pfeiffer, J. B. Stark, Q. Wu, X.-C. Zhang, and J. F. Federici, “Coherent terahertz radiation detection: Direct comparison between free-space electro-optic sampling and antenna detection,” Appl. Phys. Lett. 73, 444–446 (1998). [CrossRef]

]. The 〈110〉-oriented ZnTe crystal possesses a large electro-optic coefficient and excellent phase-matching at around 0.8 µm probe wavelength so that it is successfully used in THz time domain spectroscopy driven by Ti:sapphire lasers [7

7. Susan L. Dexheimer (Ed.), Terahertz Spectroscopy: Principles and Applications, (CRC Press, 2007). [CrossRef]

, 8

8. K. Sakai (Ed.), Terahertz Optoelectronics, (Springer Press, 2005). [CrossRef]

]. However, the detection efficiency of ZnTe deteriorates at a probe wavelength of 1.55 µm due to the phase mismatch between the optical sampling pulse and the THz radiation [9

9. L. Meignien, J. Mangeney, P. Crozat, L. Duvillaret, and M. Hanna, “Two-port vectorial terahertz electro-optic sampling system,” Appl. Phys. Lett. 92, 131103 (2007). [CrossRef]

]. A possible solution is the conversion of the electro-optic probe wavelength from 1.55 µm to 0.8 µm via second harmonic generation in nonlinear optical crystals [2

2. A. Schneider, M. Stillhart, and P. Günter, “High efficiency generation and detection of terahertz pulses using laser pulses at telecommunication wavelengths,” Opt. Express 14, 5376–5384 (2006). [CrossRef] [PubMed]

]. However, the limited conversion efficiency reduces the optical intensity available for THz sampling. Such an approach also increases the complexity of the setup. Nagai et al. [10

10. M. Nagai, K. Tanaka, H. Ohtake, T. Bessho, T. Sugiura, T. Hirosumi, and M. Yoshida, “Generation and detection of terahertz radiation by electro-optical process in GaAs using 1.56 µm fiber laser pulses,” Appl. Phys. Lett. 85, 3974–3976 (2004). [CrossRef]

] proposed 〈110〉-oriented GaAs as a substitution for ZnTe in THz spectrometers driven by fiber lasers, since the optical group velocity at 1.55 µm is closer to the THz phase velocity in GaAs than in ZnTe. Pradarutti et al. [11

11. B. Pradarutti, G. Matthäus, S. Riehemann, G. Notni, S. Nolte, and A. Tünnermann, “Highly efficient terahertz electro-optic sampling by material optimization at 1060 nm,” Opt. Commun. 281, 5031–5035 (2008). [CrossRef]

] studied the THz response in 〈110〉-oriented GaAs at 1.06 µm probe wavelength. Vossebürger et al. [12

12. M. Vossebürger, M. Brucherseifer, G. C. Cho, H. G. Roskos, and H. Kurz, “Propagation effects in electro-optic sampling of terahertz pulses in GaAs,” Appl. Opt. 37, 3368–3371 (1998). [CrossRef]

] studied the THz response in GaAs crystals of different thicknesses at 0.9 µm optical sampling wavelength. However, there is no detailed study of the thickness dependence of the THz response in 〈110〉-oriented GaAs using electro-optic sampling at 1.55 µm wavelength, which could be helpful to design commercial THz spectrometers driven by fiber lasers.

In this paper, we present a study of the THz response of 〈110〉-oriented GaAs for different crystal thicknesses in the range from 0.2 mm to 2.0 mm. To this end, we perform FSEOS in 〈110〉-oriented GaAs using a 1.55 µm femtosecond fiber laser for the sampling of a THz pulse form. The experimental results for the bandwidth response are compared with theory by modeling the frequency response function in order to identify signal features that depend on the thickness of the detection crystal. The response bandwidth is limited by the propagation velocity difference between the probe beam and the frequency components of the THz pulse. In addition to this group velocity mismatch, absorption of the THz radiation in the electro-optic crystal can have detrimental effects on the response sensitivity of FSEOS. Therefore, we also study the influence of the crystal thickness on the sampling sensitivity. We find that absorption has a negligible effect on the response sensitivity in the crystal thickness range studied here, while our theoretical model predicts strong saturation for crystal thicknesses exceeding 5 mm.

2. Experiment

We cut a 〈110〉-oriented semi-insulating GaAs crystal with a thickness of 2 mm into 10 mm × 10 mm sized pieces. Each piece is polished mechanically to different thicknesses from 2.0 mm to 0.2 mm in 0.2 mm steps. The THz pulse forms are recorded in a THz time domain spectroscopy setup. A mode-locked Er-doped fiber laser (TC-1550, MenloSystems GmbH) is used as light source. It emits pulses with 100 fs duration and 1.55 µm central wavelength at a repetition rate of 100 MHz. In our setup, the THz emitter is triggered with laser pulses of 33 mW average power, while a probe beam of 5 mW is used for FSEOS. The THz emitter consists of a photoconductive switch patterned on a 500 nm thick ErAs:In0.53Ga0.47As superlattice with 10 nm period grown on top of an InAlAs buffer layer and a semi-insulating InP substrate. The ErAs:In0.53Ga0.47As superlattice is a high performance photoconductor at 1.55 µm, with a short carrier lifetime (0.3 ps) [13

13. F. Ospald, D. Maryenko, K. von Klitzing, D. C. Driscoll, M. P. Hanson, H. Lu, A. C. Gossard, and J. H. Smet, “1.55 µm ultrafast photoconductive switches based on ErAs:InGaAs,” Appl. Phys. Lett. 92, 131117 (2008). [CrossRef]

] and a high electron Hall mobility (906 cm2/Vs) [14

14. D. C. Driscoll, M. P. Hanson, A. C. Gossard, and E. R. Brown, “Ultrafast photoresponse at 1.55 µm in InGaAs with embedded semimetallic ErAs nanoparticles,” Appl. Phys. Lett. 86, 051908 (2005). [CrossRef]

]. The antenna consists of a bow-tie geometry with an opening angle of 30° and a gap of 10 µm × 10 µm. In order to improve the signal-to-noise ratio (SNR), the photoconductive ErAs:In0.53Ga0.47As is etched away everywhere except at the center of the bow-tie antenna, which is illuminated, in order to expose the well insulating substrate and reduce the dark current [15

15. A. Schwagmann, Z.-Y. Zhao, F. Ospald, H. Lu, D. C. Driscoll, M. P. Hanson, A. C. Gossard, and J. H. Smet, “Terahertz emission characteristics of ErAs:InGaAs-based photoconductive antennas excited at 1.55 µm,” Appl. Phys. Lett. 96, 141108 (2010). [CrossRef]

]. Our emitter is biased at 20 kV/cm field using a block function voltage at a frequency of 33 KHz for lock-in amplification. A hemispherical high-resistivity silicon lens with 6 mm diameter is used to collimate the THz emission in order to improve the detection efficiency. Two off-axis parabolic mirrors focus the THz radiation on the GaAs crystal where it overlaps with the 1.55 µm probe pulse train. The electric field of the THz radiation induces birefringence in the GaAs crystal, which causes a change of the polarization state of the 1.55 µm probe beam. This change is analyzed with a quarter-wave plate, a Wollaston prism and a balanced photodetector. The THz propagation path is enclosed in a nitrogen atmosphere to avoid spectral dips induced by aqueous vapor absorption. The SNR exceeds 40 dB in our experiment.

3. Results and Discussion

Figure 1(a) shows the normalized THz pulse forms detected by GaAs crystals with thicknesses of 2.0 mm, 1.0 mm and 0.2 mm, respectively. Internal reflections at the surfaces of the GaAs crystals cause the signal echoes in the traces recorded with the 1.0 mm and 0.2 mm thick crystals. These echoes lead to frequency ripples in the THz spectra, which are obtained by Fast Fourier Transform (FFT). In order to avoid this rippling, we transform the time domain signals into frequency spectra in a selected time window excluding all the echoes. This time window is fixed for all crystal thicknesses and limited by the positions of the echoes for the thinnest crystal. The peak SNR of the spectra remains at about 40 dB. The time domain response is estimated from the full width at half maximum (FWHM) of the main positive peak of the pulse form as indicated by arrows in Fig. 1(a). When the thickness of GaAs is reduced from 2.0 mm to 0.2 mm, the FWHM decreases from 0.5 ps to 0.3 ps.

Fig. 1. (a) Normalized THz pulse forms detected by 〈110〉-oriented GaAs crystals with thicknesses of 2.0 mm, 1.0 mm, and 0.2 mm. (b) Fast Fourier Transform of the time domain data. The time window for the calculation of the spectra is equal for all spectra and restricted to avoid the inclusion of echoes.

The change of the pulse form in the time domain for different crystal thicknesses is also reflected in the frequency domain data. Figure 1(b) shows the THz spectra corresponding to the pulse forms in the time domain. The detected bandwidth is approximately equal to the reciprocal temporal FWHM and increases from 2 THz to 3.3 THz when the thickness of the GaAs crystal is reduced from 2.0 mm to 0.2 mm. However, the detected bandwidth is limited both by the emitter and the finite duration of the probe pulse as shown below.

The efficiency of the electro-optic sampling process critically depends on the fulfillment of the phase-matching condition

Δk=k(vopt+vTHz)k(vopt)k(vTHz)=0.
(1)

For the frequencies contained in the optical pulse (νopt) and the terahertz pulse (νTHz) in our experiments, νTHzνopt, which justifies the approximation

k(vopt+vTHz)k(vopt)+vTHz(kv)v=vopt.
(2)

Inserting Eq. (2) into Eq. (1), the phase-matching condition is found to be equivalent to

ngr(vopt)nph(vTHz)=0,
(3)

where n gr is the group refractive index and n ph the phase refractive index. Optimal sampling of a specific THz frequency is therefore achieved when this frequency component of the THz pulse form traverses the GaAs crystal with the same phase velocity as the group velocity of the infrared probe pulse. Velocity mismatch leads to a temporal walk-off δ after propagation through the crystal of

δ(vTHz)=ngr(vopt)nph(vTHz)cl,
(4)

where c is the speed of light in vacuum and l is the crystal thickness.

The optical group refractive index is defined as ngr(vopt)=nph(vopt)+vopt(nphvopt) and can be approximated with the Sellmeier equation [16

16. J. S. Blakemore (Ed.), Gallium Arsenide, (The American Institute of Physis, 1987).

]. In the following, we assume the probe pulse to be temporally and spectrally δ-like at a wavelength λ 0 = 1.55 µm and neglect dispersive broadening. This yields for the probe pulse a group refractive index n gr(λ 0) = 3.5. We also do not take into account absorption of the probe pulse because its photon energy is smaller than the bandgap in GaAs (E gap = 1.43 eV). In the THz range, the phase refractive index can be calculated as nph(vTHz)=ε()+ε(0)ε()1(vTHzvTO)2 , where ν TO = 8.05 THz is the TO-phonon resonance frequency and ε the frequency dependent permittivity [17

17. T. Hattori, Y. Homma, A. Mitsuishi, and M. Tacke, “Indices of refraction of ZnS, ZnSe, ZnTe, CdS, and CdTe in the far infrared,” Opt. Commun. 7, 229–232 (1973). [CrossRef]

]. The features in our experiments and simulations appear at frequencies ν THz < 6 THz, so that the phonon absorption is irrelevant here. The values for the GaAs high frequency permittivity limit ε (∞) = 10.8 and the DC permittivity ε(0) = 12.7 are best-fit values from the comparison of the distinct features in the response function and the recorded spectra. They lie within the range of measured values reported in the literature [18

18. O. Madelung, U. Rössler, and M. Schulz (Ed.), Landolt-Börnstein - Group III Condensed Matter, vol. 41A1a, (Springer Press, 2001).

]. The amplitude of the electro-optic modulation of the probe beam by an electric field of frequency νTHz is proportional to the average of the field over the mismatch time δ(ν THz), which can be expressed by the frequency response function [19

19. Q. Wu and X.-C. Zhang, “7 terahertz broadband GaP electro-optic sensor,” Appl. Phys. Lett. 70, 1784–1786 (1997). [CrossRef]

, 20

20. A. Leitenstorfer, S. Hunsche, J. Shah, M. C. Nuss, and W. H. Knox, “Detectors and sources for ultrabroadband electro-optic sampling: experiment and theory,” Appl. Phys. Lett. 74, 1516–1518 (1999). [CrossRef]

]

G(vTHz)=2nph(vTHz)+1×2(1cos(2πvTHzδ(vTHz)))2πvTHzδ(vTHz).
(5)

Fig. 2. THz frequency response of 〈110〉-oriented GaAs crystals with thicknesses of (a): 2 mm, (b): 1.6 mm, (c): 1.2 mm, (d): 1 mm, (e): 0.6 mm and (f): 0.2 mm, (λ 0 = 1.55 µm). In each panel, the upper curve is the calculated THz response, and the lower curve is the measured THz spectrum as detected with GaAs of the corresponding thickness.

Figure 3 plots the measured and calculated bandwidths for all crystal thicknesses considered in this work. It shows the excellent congruence for l ≥ 1 mm as well as the increasing discrepancy between theory and experiment for smaller l, for which the experimental bandwidth saturates. We attribute this mainly to the following two aspects: (1) the limited output bandwidth of our emitter [15

15. A. Schwagmann, Z.-Y. Zhao, F. Ospald, H. Lu, D. C. Driscoll, M. P. Hanson, A. C. Gossard, and J. H. Smet, “Terahertz emission characteristics of ErAs:InGaAs-based photoconductive antennas excited at 1.55 µm,” Appl. Phys. Lett. 96, 141108 (2010). [CrossRef]

]; and (2) the deterioration of the SNR due to the limited interaction length in thinner crystals.

ΔII=sin(2πngr3(λ0)γ41ETHzλ0l)2πngr3(λ0)γ41ETHzλ0l.
(6)

Here, γ 41 = 1.5 pm/V is the electro-optic coefficient, n gr(λ 0) = 3.5 is the group refractive index of GaAs at the optical wavelength λ 0 = 1.55 µm, and E THz is the electric field of the THz pulse form. Since γ 41 is very small, the sine can be approximated by its argument. Therefore, for a fixed electric field, the THz response sensitivity ΔI/I is proportional to the crystal thickness l. We would like to point out that this simple model so far neglects absorption of both the optical probe pulse and the THz radiation. We use near infrared (NIR) transmission spectroscopy and Fourier transform infrared (FT-IR) spectroscopy to investigate the transmission properties of GaAs in the optical and THz region, respectively. While we experimentally find its optical absorption coefficient to be negligible (α = 3 × 10−3 cm−1), the THz absorption coefficient is considerable (e.g., α THz = 5.6 cm−1 at 3 THz). These results are in good agreement with previously published data [23

23. J. Pastrňák, F. Karel, and O. Petřiček, “Optical absorption coefficient of semiconductors in the extrinsic region obtained by photoconductivity measurements: application to SI GaAs,” Semicond. Sci. Technol. 5, 867–870 (1990). [CrossRef]

, 24

24. R. H. Stolen, “Far-infrared absorption in high resistivity GaAs,” Appl. Phys. Lett. 15, 74–75 (1969). [CrossRef]

]. In order to account for the absorption of the THz radiation in the GaAs crystal, we replace the static term E THz · l in Eq. (6) by

Fig. 3. Bandwidth as a function of thickness: Discs: measured data; solid line: cut-off frequency calculated according to the frequency response function [Eq. (5)].
0lETHz(z)dz=0lE0·exp(αTHz·z)dz.
(7)

Here, the attenuation of E 0, the THz electric field incident on the electro-optic crystal, in dependence of the penetration depth z, is described with the Lambert-Beer law (see also the inset of Fig. 4). For the sake of completeness, note that we also lump the partial reflection of the THz field at the crystal surface into E 0, which will be used as a fit parameter in the corrected THz response sensitivity

ΔII=4πE0ngr3(λ0)γ41(1exp(αTHz·l2))αTHz·λ0.
(8)

We would like to point out that this equation reduces to Eq. (6) when α THz approaches zero. The inclusion of the absorption of the THz radiation in the model leads to a sublinear dependence of the THz response sensitivity on l, as intuitively expected.

Figure 4 plots the measured and fitted THz response sensitivity as a function of thickness. We use the incident THz electric field E 0 = 20.6 V/cm as a fit parameter and the experimentally obtained THz absorption coefficient of α THz = 5.6 cm−1 as mean value in our range of THz frequencies. The fitted values match our experimental results within the error bars. However, the sublinearity due to absorption in the thickness range of up to 2 mm is found to be negligible. The simulation of the THz electro-optic sampling sensitivity predicts stronger saturation effects for a crystal thickness range beyond the experimentally studied thicknesses. For example, at l = 5 mm, already 75% of the theoretical maximum sensitivity are reached, and a 10 mm thick crystal would exhibit 94% sensitivity.

Fig. 4. THz electro-optic sampling sensitivity as a function of thickness. Discs: experimental data; dashed line: fit without THz absorption according to Eq. (6); solid line: fit including THz absorption according to Eq. (8). Inset: schematic of the THz attenuation inside a GaAs crystal.

4. Conclusion

In summary, we have studied the THz response bandwidth and sensitivity of FSEOS in 〈110〉-oriented GaAs at a probe wavelength of 1.55 µm for different crystal thicknesses. The measured THz response bandwidths are compared to a basic frequency response function. The cut-off frequencies are in very good agreement for crystal thicknesses l ≥ 1 mm, supporting the usability of the model. A crystal with a thickness of 0.2 mm was successfully employed for FSEOS. Limitations in the emitter bandwidth and the finite optical pulse duration prevented to experimentally demonstrate the theoretically predicted response bandwidth of up to 5 THz. Moreover, the effects of the absorption of the THz radiation in the electro-optic crystal on the detection sensitivity were studied. While in our crystal thickness range absorption was found to have no considerable detrimental effect on the response sensitivity, the model predicts strong saturation of the sensitivity for crystal thicknesses exceeding 5 mm.

Acknowledgments

The authors would like to thank M. Theuer and C. Petermann for helpful discussions regarding the setup and acknowledge financial support from the TEKZAS project (Grant No. 13N9471) and the NanoFutur Young Investigator Award of the German Ministry of Science and Education (Grant No. 03X5503A). A. S. is grateful for support from the Thomas Gessmann-Foundation.

References and links

1.

B. Sartorius, H. Roehle, H. Künzel, J. Böttcher, M. Schlak, D. Stanze, H. Venghaus, and M. Schell, “All-fiber terahertz time-domain spectrometer operating at 1.5 µm telecom wavelengths,” Opt. Express 16, 9565–9570 (2008). [CrossRef] [PubMed]

2.

A. Schneider, M. Stillhart, and P. Günter, “High efficiency generation and detection of terahertz pulses using laser pulses at telecommunication wavelengths,” Opt. Express 14, 5376–5384 (2006). [CrossRef] [PubMed]

3.

J. Mangeney and P. Crozat, “Ion-irradiated In0.53Ga0.47As photoconductive antennas for THz generation and detection at 1.55 µm wavelength,” C. R. Phys. 9, 142–152 (2008). [CrossRef]

4.

A. Takazato, M. Kamakura, T. Matsui, J. Kitagawa, and Y. Kadoya, “Terahertz wave emission and detection using photoconductive antennas made on low-temperature-grown InGaAs with 1.56 µm pulse excitation,” Appl. Phys. Lett. 91, 011102 (2007). [CrossRef]

5.

H. Roehle, R. J. B. Dietz, H. J. Hensel, J. Böttcher, H. Künzel, D. Stanze, M. Schell, and B. Sartorius, “Next generation 1.5 µm terahertz antennas: mesa-structuring of InGaAs/InAlAs photoconductive layers,” Opt. Express 18, 2296–2301 (2010). [CrossRef] [PubMed]

6.

Y. Cai, I. Brener, J. Lopata, J. Wynn, L. Pfeiffer, J. B. Stark, Q. Wu, X.-C. Zhang, and J. F. Federici, “Coherent terahertz radiation detection: Direct comparison between free-space electro-optic sampling and antenna detection,” Appl. Phys. Lett. 73, 444–446 (1998). [CrossRef]

7.

Susan L. Dexheimer (Ed.), Terahertz Spectroscopy: Principles and Applications, (CRC Press, 2007). [CrossRef]

8.

K. Sakai (Ed.), Terahertz Optoelectronics, (Springer Press, 2005). [CrossRef]

9.

L. Meignien, J. Mangeney, P. Crozat, L. Duvillaret, and M. Hanna, “Two-port vectorial terahertz electro-optic sampling system,” Appl. Phys. Lett. 92, 131103 (2007). [CrossRef]

10.

M. Nagai, K. Tanaka, H. Ohtake, T. Bessho, T. Sugiura, T. Hirosumi, and M. Yoshida, “Generation and detection of terahertz radiation by electro-optical process in GaAs using 1.56 µm fiber laser pulses,” Appl. Phys. Lett. 85, 3974–3976 (2004). [CrossRef]

11.

B. Pradarutti, G. Matthäus, S. Riehemann, G. Notni, S. Nolte, and A. Tünnermann, “Highly efficient terahertz electro-optic sampling by material optimization at 1060 nm,” Opt. Commun. 281, 5031–5035 (2008). [CrossRef]

12.

M. Vossebürger, M. Brucherseifer, G. C. Cho, H. G. Roskos, and H. Kurz, “Propagation effects in electro-optic sampling of terahertz pulses in GaAs,” Appl. Opt. 37, 3368–3371 (1998). [CrossRef]

13.

F. Ospald, D. Maryenko, K. von Klitzing, D. C. Driscoll, M. P. Hanson, H. Lu, A. C. Gossard, and J. H. Smet, “1.55 µm ultrafast photoconductive switches based on ErAs:InGaAs,” Appl. Phys. Lett. 92, 131117 (2008). [CrossRef]

14.

D. C. Driscoll, M. P. Hanson, A. C. Gossard, and E. R. Brown, “Ultrafast photoresponse at 1.55 µm in InGaAs with embedded semimetallic ErAs nanoparticles,” Appl. Phys. Lett. 86, 051908 (2005). [CrossRef]

15.

A. Schwagmann, Z.-Y. Zhao, F. Ospald, H. Lu, D. C. Driscoll, M. P. Hanson, A. C. Gossard, and J. H. Smet, “Terahertz emission characteristics of ErAs:InGaAs-based photoconductive antennas excited at 1.55 µm,” Appl. Phys. Lett. 96, 141108 (2010). [CrossRef]

16.

J. S. Blakemore (Ed.), Gallium Arsenide, (The American Institute of Physis, 1987).

17.

T. Hattori, Y. Homma, A. Mitsuishi, and M. Tacke, “Indices of refraction of ZnS, ZnSe, ZnTe, CdS, and CdTe in the far infrared,” Opt. Commun. 7, 229–232 (1973). [CrossRef]

18.

O. Madelung, U. Rössler, and M. Schulz (Ed.), Landolt-Börnstein - Group III Condensed Matter, vol. 41A1a, (Springer Press, 2001).

19.

Q. Wu and X.-C. Zhang, “7 terahertz broadband GaP electro-optic sensor,” Appl. Phys. Lett. 70, 1784–1786 (1997). [CrossRef]

20.

A. Leitenstorfer, S. Hunsche, J. Shah, M. C. Nuss, and W. H. Knox, “Detectors and sources for ultrabroadband electro-optic sampling: experiment and theory,” Appl. Phys. Lett. 74, 1516–1518 (1999). [CrossRef]

21.

H. J. Bakker, G. C. Cho, H. Kurz, Q. Wu, and X.-C. Zhang, “Distortion of terahertz pulses in electro-optic sampling,” J. Opt. Soc. Am. B 15, 1795–1801 (1998). [CrossRef]

22.

P. C. M. Planken, C. E. W. M. van Rijmenam, and R. N. Schouten, “Opto-electronic pulsed THz systems,” Semicond. Sci. Technol. 20, S121–S127 (2005). [CrossRef]

23.

J. Pastrňák, F. Karel, and O. Petřiček, “Optical absorption coefficient of semiconductors in the extrinsic region obtained by photoconductivity measurements: application to SI GaAs,” Semicond. Sci. Technol. 5, 867–870 (1990). [CrossRef]

24.

R. H. Stolen, “Far-infrared absorption in high resistivity GaAs,” Appl. Phys. Lett. 15, 74–75 (1969). [CrossRef]

OCIS Codes
(230.2090) Optical devices : Electro-optical devices
(300.6495) Spectroscopy : Spectroscopy, teraherz
(060.3510) Fiber optics and optical communications : Lasers, fiber

ToC Category:
Spectroscopy

History
Original Manuscript: May 20, 2010
Revised Manuscript: June 28, 2010
Manuscript Accepted: June 28, 2010
Published: July 13, 2010

Citation
Zhenyu Zhao, Andre Schwagmann, Frank Ospald, Daniel C. Driscoll, Hong Lu, Arthur C. Gossard, and Jurgen H. Smet, "Thickness dependence of the terahertz response in 〈110〉-oriented GaAs crystals for electro-optic sampling at 1.55 µm," Opt. Express 18, 15956-15963 (2010)
http://www.opticsinfobase.org/oe/abstract.cfm?URI=oe-18-15-15956


Sort:  Author  |  Year  |  Journal  |  Reset  

References

  1. B. Sartorius, H. Roehle, H. Künzel, J. Böttcher, M. Schlak, D. Stanze, H. Venghaus, and M. Schell, “All-fiber terahertz time-domain spectrometer operating at 1.5 μm telecom wavelengths,” Opt. Express 16, 9565–9570 (2008). [CrossRef] [PubMed]
  2. A. Schneider, M. Stillhart, and P. Günter, “High efficiency generation and detection of terahertz pulses using laser pulses at telecommunication wavelengths,” Opt. Express 14, 5376–5384 (2006). [CrossRef] [PubMed]
  3. J. Mangeney, and P. Crozat, “Ion-irradiated In0.53Ga0.47As photoconductive antennas for THz generation and detection at 1.55 μm wavelength,” C. R. Phys. 9, 142–152 (2008). [CrossRef]
  4. A. Takazato, M. Kamakura, T. Matsui, J. Kitagawa, and Y. Kadoya, “Terahertz wave emission and detection using photoconductive antennas made on low-temperature-grown InGaAs with 1.56 μm pulse excitation,” Appl. Phys. Lett. 91, 011102 (2007). [CrossRef]
  5. H. Roehle, R. J. B. Dietz, H. J. Hensel, J. Böttcher, H. Künzel, D. Stanze, M. Schell, and B. Sartorius, “Next generation 1.5 μm terahertz antennas: mesa-structuring of InGaAs/InAlAs photoconductive layers,” Opt. Express 18, 2296–2301 (2010). [CrossRef] [PubMed]
  6. Y. Cai, I. Brener, J. Lopata, J. Wynn, L. Pfeiffer, J. B. Stark, Q. Wu, X.-C. Zhang, and J. F. Federici, “Coherent terahertz radiation detection: Direct comparison between free-space electro-optic sampling and antenna detection,” Appl. Phys. Lett. 73, 444–446 (1998). [CrossRef]
  7. S. L. Dexheimer, ed., Terahertz Spectroscopy: Principles and Applications, (CRC Press, 2007) [CrossRef]
  8. K. Sakai, ed., Terahertz Optoelectronics, (Springer Press, 2005) [CrossRef]
  9. L. Meignien, J. Mangeney, P. Crozat, L. Duvillaret, and M. Hanna, “Two-port vectorial terahertz electro-optic sampling system,” Appl. Phys. Lett. 92, 131103 (2007). [CrossRef]
  10. M. Nagai, K. Tanaka, H. Ohtake, T. Bessho, T. Sugiura, T. Hirosumi, and M. Yoshida, “Generation and detection of terahertz radiation by electro-optical process in GaAs using 1.56 μm fiber laser pulses,” Appl. Phys. Lett. 85, 3974–3976 (2004). [CrossRef]
  11. B. Pradarutti, G. Matthäus, S. Riehemann, G. Notni, S. Nolte, and A. Tünnermann, “Highly efficient terahertz electro-optic sampling by material optimization at 1060 nm,” Opt. Commun. 281, 5031–5035 (2008). [CrossRef]
  12. M. Vossebürger, M. Brucherseifer, G. C. Cho, H. G. Roskos, and H. Kurz, “Propagation effects in electro-optic sampling of terahertz pulses in GaAs,” Appl. Opt. 37, 3368–3371 (1998). [CrossRef]
  13. F. Ospald, D. Maryenko, K. von Klitzing, D. C. Driscoll, M. P. Hanson, H. Lu, A. C. Gossard, and J. H. Smet, “1.55 μm ultrafast photoconductive switches based on ErAs:InGaAs,” Appl. Phys. Lett. 92, 131117 (2008). [CrossRef]
  14. D. C. Driscoll, M. P. Hanson, A. C. Gossard, and E. R. Brown, “Ultrafast photo response at 1.55 μm in InGaAs with embedded semimetallic ErAs nanoparticles,” Appl. Phys. Lett. 86, 051908 (2005). [CrossRef]
  15. A. Schwagmann, Z.-Y. Zhao, F. Ospald, H. Lu, D. C. Driscoll, M. P. Hanson, A. C. Gossard, and J. H. Smet, “Terahertz emission characteristics of ErAs:InGaAs-based photoconductive antennas excited at 1.55 μm,” Appl. Phys. Lett. 96, 141108 (2010). [CrossRef]
  16. J. S. Blakemore, ed., Gallium Arsenide, (The American Institute of Physics, 1987)
  17. T. Hattori, Y. Homma, A. Mitsuishi, and M. Tacke, “Indices of refraction of ZnS, ZnSe, ZnTe, CdS, and CdTe in the far infrared,” Opt. Commun. 7, 229–232 (1973). [CrossRef]
  18. O. Madelung, U. Rössler, and M. Schulz, eds., Landolt-Börnstein - Group III Condensed Matter, (Springer Press, 2001) Vol. 41A1a
  19. Q. Wu, and X.-C. Zhang, “7 terahertz broadband GaP electro-optic sensor,” Appl. Phys. Lett. 70, 1784–1786 (1997). [CrossRef]
  20. A. Leitenstorfer, S. Hunsche, J. Shah, M. C. Nuss, and W. H. Knox, “Detectors and sources for ultra broadband electro-optic sampling: experiment and theory,” Appl. Phys. Lett. 74, 1516–1518 (1999). [CrossRef]
  21. H. J. Bakker, G. C. Cho, H. Kurz, Q. Wu, and X.-C. Zhang, “Distortion of terahertz pulses in electro-optic sampling,” J. Opt. Soc. Am. B 15, 1795–1801 (1998). [CrossRef]
  22. P. C. M. Planken, C. E. W. M. van Rijmenam, and R. N. Schouten, “Opto-electronic pulsed THz systems,” Semicond. Sci. Technol. 20, S121–S127 (2005). [CrossRef]
  23. J. Pastrňák, F. Karel, and O. Petřiček, “Optical absorption coefficient of semiconductors in the extrinsic region obtained by photoconductivity measurements: application to SI GaAs,” Semicond. Sci. Technol. 5, 867–870 (1990). [CrossRef]
  24. R. H. Stolen, “Far-infrared absorption in high resistivity GaAs,” Appl. Phys. Lett. 15, 74–75 (1969). [CrossRef]

Cited By

Alert me when this paper is cited

OSA is able to provide readers links to articles that cite this paper by participating in CrossRef's Cited-By Linking service. CrossRef includes content from more than 3000 publishers and societies. In addition to listing OSA journal articles that cite this paper, citing articles from other participating publishers will also be listed.

Figures

Fig. 1. Fig. 2. Fig. 3.
 
Fig. 4.
 

« Previous Article  |  Next Article »

OSA is a member of CrossRef.

CrossCheck Deposited